1. Ingot heating
For extrusion production, extrusion temperature is the most basic and most critical process factor. Extrusion temperature has a great influence on product quality, production efficiency, die life, energy consumption, etc.
The most important problem of extrusion is the control of the metal temperature. From the heating of the ingot to the quenching of the extruded profile, it is necessary to ensure that the soluble phase structure does not precipitate from the solid solution or shows the dispersion of small particles.
The heating temperature of 6063 alloy ingot is generally set within the temperature range of Mg2Si precipitation. The heating time has an important influence on the precipitation of Mg2Si. Rapid heating can greatly reduce the possible precipitation time. Generally speaking, the heating temperature of 6063 alloy ingot can be set as: non-homogenized ingot: 460-520℃; homogenized ingot: 430-480℃.
The extrusion temperature is adjusted according to different products and unit pressure during operation. During the extrusion process, the temperature of the ingot in the deformation zone changes. With the completion of the extrusion process, the temperature of the deformation zone gradually increases, and it increases with the increase of the extrusion speed. Therefore, in order to prevent extrusion cracks, as the extrusion process progresses and the temperature of the deformation zone increases, the extrusion speed should be gradually reduced.
2. Control the extrusion speed of aluminum
The extrusion speed must be carefully controlled during the extrusion process. Extrusion speed has an important influence on deformation heat effect, deformation uniformity, recrystallization and solid solution process, product mechanical properties and product surface quality.
If the extrusion speed is too fast, pitting and cracks will appear on the surface of the product. At the same time, the extrusion speed is too fast to increase the unevenness of the metal deformation. The flow rate during extrusion depends on the alloy type and the geometry, size and surface condition of the profile.
The extrusion speed of 6063 alloy profile (the outflow speed of metal) can be selected from 20-100 m/min.
With the advancement of modern technology, the extrusion speed can be controlled by program or simulation program. At the same time, new technologies such as isothermal extrusion process and CADEX have also been developed. By automatically adjusting the extrusion speed to keep the temperature of the deformation zone within a certain constant range, the purpose of rapid extrusion without cracks can be achieved.
In order to improve production efficiency, many measures can be taken in the process. When induction heating is used, there is a temperature gradient of 40-60°C (gradient heating) along the length of the ingot. During extrusion, the high temperature end faces the extrusion die and the low temperature end faces the extrusion pad to balance a part of the deformation heat; Water-cooled die extrusion, that is, forced cooling by passing water at the back end of the mold, the test proves that the extrusion speed can be increased by 30%-50%.
In recent years, nitrogen or liquid nitrogen is used to cool the mold (extrusion mold) abroad to increase the extrusion speed, increase the life of the mold and improve the surface quality of the profile. In the extrusion process, the nitrogen is introduced to the outlet of the extrusion die to release it, which can rapidly shrink the product to be cooled, cool the extrusion die and the metal in the deformation zone, so that the deformation heat is taken away, and at the same time the mold outlet is affected by the nitrogen atmosphere. Control, reduce the oxidation of aluminum, reduce the adhesion and accumulation of alumina, so the cooling of nitrogen improves the surface quality of the product, which can greatly increase the extrusion speed. CADEX is a newly developed extrusion process. The extrusion temperature, extrusion speed and extrusion force in the extrusion process form a closed loop system to maximize the extrusion speed and production efficiency while ensuring the best Performance.
3. On-machine quenching
6063-T5 quenching is to remove the Mg2Si solid-dissolved in the base metal at a high temperature and then quickly cool it to room temperature and be retained. The cooling rate is often proportional to the strengthening phase content. The minimum cooling rate that 6063 alloy can be strengthened is 38°C/min, so it is suitable for air quenching. Changing the number of fan and fan rotation can change the cooling intensity, so that the temperature of the product before tension straightening drops to below 60°C.
4. Tension straightening
After the profile is out of the die hole, it is generally pulled by a tractor. When the traction machine is working, it applies a certain traction tension to the extruded product and moves synchronously with the flow rate of the product. The purpose of using the traction machine is to reduce the uneven length and scratches during multi-line extrusion, and at the same time prevent the profile from twisting and bending after the die hole, which brings trouble to the tension straightening. Tension straightening can not only eliminate the longitudinal shape irregularities of the product, but also reduce its residual stress, improve the strength characteristics and maintain its good surface.
5. Artificial aging of aluminum
The aging treatment requires uniform temperature and the temperature difference does not exceed ±3-5℃. The artificial aging temperature of 6063 alloy is generally 200℃. The aging holding time is 1-2 hours. In order to improve the mechanical properties, aging at 180-190℃ is also used for 3-4 hours, but the production efficiency will be reduced at this time.